Cavity Filling Instabilities and the Accuracy of Moldflow Predictions
How do melt rheology and local shear loading affect cavity-filling quality and the reliability of Moldflow predictions?
How shear loading, rheological data and feed-system geometry affect cavity filling, Moldflow pressure predictions and jetting in injection molding.
Introduction
A cavity can fill completely and still produce a part with a surface defect or reduced durability. The reason may lie in the history of the melt as it passes through the feed system and cavity. Flow, shear deformation and heating occur together, with the most severe loading often concentrated in a gate, an abrupt transition or a thin rib. A satisfactory filling result therefore does not, on its own, establish that the material has been processed under suitable conditions.
The engineering task is to connect local flow conditions with material behavior and part performance. This paper examines that connection through shear rate, wall shear stress and the rheological data used in Moldflow. It also considers why predicted pressure may differ from machine measurements and how jetting can arise either at the gate or further along the cavity. The aim is to turn simulation results into decisions about part design, the feed system and the injection-velocity profile.
1 What Rheology Tells Us About Filling
Flow resistance is not a fixed property of a polymer melt. It changes with the conditions the material experiences along the flow path. Shear viscosity η describes this resistance at a particular temperature, shear rate and pressure. Shear rate γ̇, expressed in s⁻¹, is the velocity gradient across the thickness of the flowing layer. Shear stress τ, expressed in Pa or MPa, is the tangential loading acting within that layer. In simple shear flow, these quantities are related by τ = η · γ̇. During cavity filling, each varies with both position and time.

This relationship explains a common processing tradeoff. Most polymer melts are pseudoplastic, or shear-thinning: increasing shear rate reduces their apparent viscosity. A higher injection velocity can consequently help the melt reach a remote cavity region, while exposing the gate to greater local shear loading. Temperature generally reduces viscosity, whereas pressure can increase it. These responses depend on the commercial grade, not just the polymer family. A designation such as PA6 or PP is therefore insufficient to characterize filling behavior.
The useful question is not simply whether increasing injection velocity will improve filling. It is where the resulting change in flow resistance and shear loading will occur. An adjustment that eliminates a short shot may introduce excessive loading at the smallest cross-section. The filling pattern and the local material conditions need to be assessed together.
2 Finding Excessive Shear and Checking for Material Damage
Start by examining the restrictions along the entire flow path. Tunnel gates, narrow runners, thin ribs and abrupt reductions in cross-section are typical locations for high shear rate. The machine-to-mold interface belongs in this assessment as well. Misalignment between the nozzle and sprue bushing, or a sharp edge at their junction, can create a local peak outside the region covered by a cavity-only model.
In the example in Fig. 2, the calculated shear rate in the gate reached approximately 108,000 s⁻¹. The general shear-rate limit for PA6 is 60,000 s⁻¹. The limit for the specific material grade must be obtained and compared with the local maximum during the filling stage being assessed.

A longer filling time or a larger effective gate cross-section may bring the shear rate down. Neither adjustment can be judged at the gate alone. Slowing the flow gives the melt front more time to cool and may compromise a remote feature; changing the gate affects pressure loss, the gate vestige and potentially part removal. The revised conditions must therefore be checked against the requirements of the whole part.
If polymer degradation is suspected during actual injection molding, the incoming pellets can be compared with polymer that has already undergone the complete molding cycle, using a sample taken from the molded part. For suitable soluble materials, solution viscometry can be used to determine the limiting viscosity number, also known as intrinsic viscosity, according to the applicable procedure. A decrease relative to the incoming material may indicate a reduction in average molecular weight. By itself, however, this does not identify where or why the damage occurred: drying, plasticization, melt residence time, temperature history and any regrind content must also be considered. The limiting viscosity number is a measured polymer property, not a “shear-rate limit”.
3 Wall Shear Stress and Part Durability
Wall shear stress helps identify regions where the melt experiences high loading near the mold surface. Local peaks may be associated with thin walls, abrupt transitions or a high injection velocity. Their engineering significance depends on the specific polymer, the reliability of the input data and the quality required from the part. Comparing a predicted maximum with a general limit is useful for screening, but a pass-or-fail reading of that comparison may conceal the conditions that matter in service.
The examples in Fig. 3 show predicted wall shear stress for two different parts made from different materials, each with its own limits. Both examples lead to the same conclusion: assess the specific material and the critical location in the particular part.

High loading of the polymer melt during injection molding contributes to orientation of the internal structure and increased residual stress in the molded part, and may impair its mechanical properties. If the part is subsequently subjected to mechanical loading or comes into contact with an aggressive medium, such as gasoline, an alkali, oil or an acid, cracks may develop through environmental stress cracking (ESC). The occurrence of ESC does not, by itself, prove that the shear-stress limit was exceeded during filling. It shows only that the combined conditions—processing history, polymer selection and loading of the molded part—exceed the material’s resistance under those conditions. In practice, investigating a cracking part requires flow analysis and an assessment of melt loading during injection molding to be combined with part testing under service or assembly conditions. This means determining whether excessive shear stress or shear rate during filling reduced the performance of the molded part.
4 Why Predicted Pressure May Differ from Measurements
The quality of a pressure prediction begins with the material description. MFR and MVR—the melt flow rate and melt volume rate—are useful comparative measurements at a specified temperature and load, but neither describes a complete viscosity curve. Materials with the same flow index may have different viscosities at the shear rates encountered during filling. Simulation requires measurements across a wider range of shear rates and temperatures. Capillary rheometry covers the higher range; rotational rheometry covers the lower range. The Cross-WLF model in Autodesk Moldflow provides the mathematical description of these measured curves and their dependence on temperature and pressure.

The pressure dependence of viscosity can be important. For the thin-walled part in Fig. 5, using different pressure-dependent material data changed the predicted pressure from approximately 65 to 79 MPa. For a thicker part with lower pressure, the difference was substantially smaller. When comparing predicted injection pressure with the actual pressure measured on the machine, the location must also be defined: melt pressure at the screw, pressure in the nozzle or pressure in the cavity. The simulation inputs are also important, including whether the complete runner system has been modeled.

The next question is which parts of the flow path the model includes. Machine pressure must overcome the resistance of the nozzle and feed system as well as the cavity. A cavity model with a simplified inlet cannot account for every one of those pressure losses. Fig. 6 illustrates the effect: the predicted difference between the versions without and with the complete feed system is approximately 600 bar. The nozzle interface and inlet geometry also matter when establishing a meaningful comparison.

In narrow sections, mechanical energy dissipation may increase the local melt temperature and thereby change viscosity. Fig. 7 shows a local temperature of approximately 340 °C in a polycarbonate part with a melt-temperature setting of around 300 °C. These values alone do not confirm thermal degradation: the specific material, exposure time and temperature history are decisive.

Before attributing a discrepancy to the simulation model, check the chain of assumptions that produced the result: the exact material grade and rheological data, the extent of the modeled flow path, mesh resolution in critical regions, actual temperature and injection-velocity profiles, and the location of the pressure sensor. The velocity-to-pressure switchover is part of this check. An early transition to packing-pressure control can lower the apparent pressure peak while changing the way the remaining cavity fills and the local loading of the melt.
5 Jetting at the Gate and Within the Cavity
Jetting is a loss of controlled melt deposition. Instead of promptly contacting the cavity wall and spreading across it, a narrow stream enters an open region and is laid down irregularly. The following melt surrounds this stream, leaving a snake-like line or streak on the appearance surface. In other cases, the stream becomes completely embedded and the surface gives no obvious warning. Weld lines and trapped air within that region can nevertheless weaken the part. A gate directed along an open cavity region is particularly susceptible because the emerging stream has no immediate wall contact.

For jetting at the gate, examine the stream direction, gate cross-section and initial injection velocity together. Directing the stream toward a nearby wall, relocating the gate or reducing the initial velocity may establish a more stable filling pattern. The remedy must still allow the rest of the cavity to fill: premature freezing, weld lines, short shots and other defects remain part of the assessment.
The gate is the most critical location for jetting, but a restriction inside the part can produce a similar condition. In Fig. 9, the melt passes through a narrow arm before entering a wider region beneath the appearance surface. An unsuitable injection velocity left visible flow marks. Increasing wall thickness offers one possible remedy, with the associated risk of sink marks on the appearance surface. An increasing injection-velocity profile offers another: pass through the critical section slowly, then accelerate once the melt front has stabilized. The timing of that change should follow melt-front position, part geometry, quality requirements and the polymer used. Its consequences for the remaining flow path must also be evaluated.

6 Conclusion
A maximum value becomes useful only when it is connected to a location, a material and a processing history. Shear rate identifies critical restrictions, wall shear stress describes local loading, and the rheological model translates the imposed conditions into flow and pressure predictions. None of these results should be interpreted independently of part and gate geometry or the loading the molded part will encounter in use.
Begin a defect investigation where the problem develops, then follow the flow path back toward the machine. A local reduction in velocity, a gate change or a revised injection profile may improve the surface or reduce material loading, but each intervention also changes filling, temperature and pressure loss elsewhere. The strongest basis for a decision is agreement between the simulated flow history, measurements from the process and the behavior of the molded part and mold. That connection makes the analysis useful for engineering rather than merely for producing a successful filling result.
Related webinar
3 – Cavity filling instability, rheology, shear stress, accuracy of Moldflow results, uneven cavity filling
Frequently asked questions
Why can faster injection improve filling while increasing the risk of material damage?
Most polymer melts are shear-thinning: their apparent viscosity decreases as shear rate increases. A higher injection velocity may therefore reduce flow resistance, while increasing local shear loading in a narrow gate or thin cavity region. An improvement in filling should be assessed together with shear rate, shear stress and local melt temperature.
How can excessive shear rate be reduced without compromising part quality?
Possible measures include a longer filling time, a revised injection-velocity profile or a larger effective gate cross-section. Each change requires reassessment of the whole part. Slower filling allows more cooling of the melt front and can compromise remote features. Gate changes also affect pressure loss, the gate vestige and potentially part removal.
How can suspected polymer degradation during molding be investigated?
For suitable soluble materials, solution viscometry can compare the limiting viscosity number, or intrinsic viscosity, of incoming pellets with a sample from the molded part. A decrease may indicate reduced average molecular weight. It does not identify the cause on its own: drying, plasticization, melt residence time, temperature history and regrind content should also be investigated.
What should be checked when predicted Moldflow pressure differs from machine measurements?
Check the exact material grade and rheological data, the modeled flow path including the feed system, mesh resolution in critical regions, and the actual temperature and injection-velocity profiles. Establish where pressure is measured: melt pressure at the screw, nozzle pressure and cavity pressure are not interchangeable. Pressure-dependent viscosity and the velocity-to-pressure switchover can also contribute to the difference.
Can local melt temperature exceed the temperature setting?
Yes. Mechanical energy dissipation in narrow sections can raise the local melt temperature and change viscosity. The paper describes a polycarbonate example with a local temperature of approximately 340 °C at a melt-temperature setting of around 300 °C. That value alone does not establish degradation: the material grade, exposure time and temperature history are decisive.
Can jetting develop inside the cavity, and how can it be controlled?
Yes. Melt emerging from a narrow arm into a wider cavity region can form an unstable stream. Geometry changes or an increasing injection-velocity profile may help: pass through the critical section slowly, then accelerate after the melt front stabilizes. Increasing wall thickness can also increase sink marks. For jetting at the gate, assess gate orientation and whether the stream can be directed toward a nearby wall.